Pulsed Plasma-Pulsed GTA Arc : a study of the process variables
A complete evaluation of the pulse parameters for the Plasma-Arc Welding (PAW) and Gas Tungsten-Arc Welding (GTAW) processes was conducted. The pulse parameters evaluated were: the background current (IB), the peak current (Ip), the average current (Iav), the RMS current (IRMS), the pulse time ratio (tp/tB), the pulse wave form and the pulse frequency (Hz). Both low (one-forty Hz) and high (two-twenty kHz) pulse frequencies were evaluated. High frequency was also superimposed on low frequency for the pulsed GTAW process. Comparisons of constant and pulsed current plasma welds were made for the melt-in, full penetration and keyhole modes of welding. For contrast, constant and pulsed current GTA welds were made under the same welding conditions of the plasma welds. Two plasma welding systems with different torch design and a GTA welding system were utilized and compared in this investigation. The material used was 0.109 inches thick Inconel 600 alloy sheets.
Optimum pulse welding conditions for both the PAW and GTAW processes were determined. The average current was found to be the controlling pulse welding parameter for both the PAW and GTAW processes. The background current was found to be optimum when it is the minimum melting current level for a given set of pulsed plasma-arc welding conditions. For this background current, the energy input was the lowest compared to all other pulse settings at the same average current. For the pulsed GTAw process with the given average current the lowest background current with the longest pulse duration (high pulse time ratio (tp/tB) was found to be optimum. For contrast, the highest peak current at shortest pulse duration was found to be optimum for a given average current with the pulsed plasma process.
In general, it was found that for both the PAW and the GTAW processes, the lower the pulse frequency, the narrower the HAZ and the wider the fusion zone. At higher pulse frequencies, however, the HAZ became wider while the fusion zone became narrower, indicating a decrease in melting efficiency at higher pulse frequencies. Neither the high frequency pulsing of PAW or the GTAW processes, nor the superimposed high frequency on the low frequency pulsing resulted in any significant improvement in the weld bead configuration or microstructure.
The microstructural observations made in this study further illustrated an important aspect of the solidification process in welds. It was observed that the partially melting region (liquidus-solidus region) immediately adjacent to the fusion line often exhibited a grain size smaller than that of the HAZ region adjacent to it but slightly further away from the fusion line. A theory regarding the effect of the partially melted region on the weld fusion zone grain size and the possibility of influencing control over the grain size and shape by the pulsed current mode is postulated.
Thesis75.O527.pdf
12.08 MB
Adobe PDF
251073b46bd0b938c3203e18d20f5fa3