On the thermal cycling of aluminum matrix composite materials
Various 606l aluminum matrix composite materials were thermally cycled from room temperature to 425°C. The materials were reinforced with stainless steel, silicon carbide, and boron fibers. The mechanical properties that were investigated included longitudinal and transverse modulus, longitudinal and transverse ultimate tensile strength, Poisson's ratio, and density. The total heating and cooling cyclic period was varied from three to six to twelve minutes per cycle, and then the room temperature mechanical properties were compared to those obtained from the as-received material. The thermal expansion of the boron-aluminum composite was measured during the thermal cycling process for each of the cyclic periods.
It was observed that the matrix sustained damage during the thermal cycling in all of the materials. The damage was in the form of cracks and voids. The matrix damage increased with cyclic period. There was degradation in the tensile and transverse strength for all of the thermally cycled materials. . The degradation of the composite strength was more severe in the boron-aluminum material than in the other materials investigated. The strength reduction in boron-aluminum became more pronounced as the cyclic period increased. The elastic modulus of some of the thermally cycled material decreased. Metallographic observations of thermally fatigued material produced evidence of grain boundary movement. The thermal expansion results indicated that by increasing the cyclic period, the maximum extension during one cycle decreased.
The results of the investigation of the composites' strengths were explained in terms of the degradation of the fiber-matrix bond. Since a unique strength value cannot be assigned to the brittle boron and silicon carbide fibers, the theoretical prediction of the tensile strength of the composite reinforced with these fibers was discussed using a range of values defined by an upper and lower strength limit. The lower limit was predicted from a model with a weak interfacial bond, and a strong bond was assumed in calculating an upper limit. It was concluded that the thermal cycling process deteriorated the fiber-matrix bond.
The extension of the boron-aluminum material during thermal cycling was observed to be controlled by the matrix at the lower temperatures during the thermal fatigue process. As the temperature increased, the stresses acting on the fibers due to the greater thermal expansion of the matrix were reduced. As the cyclic period increased, the stresses acting on the fibers were relaxed, and the thermal expansion of the composite was dominated by the thermal expansion of the fiber.
Thesis75.H644.pdf
12.14 MB
Adobe PDF
2dbf3064d788d43e634eca49fa808824