The effect of environment on thermal cycling damage in boron-aluminum composites
Boron-aluminum composites having 6061, 2024, and 1100 alloy matrices were subjected to 6,000 thermal cycles between ambient temperature and 425°C in argon and in air. Both longitudinally and transversely oriented specimens were used. Cycling in argon was performed using periods of six and twelve minutes per cycle. The cyclic period used in air was twelve minutes per cycle. The strength, stiffness, and Poisson's ratio properties were measured after cycling and compared to the same properties in the as-fabricated condition. Also, the strengths of fibers extracted from both cycled and uncycled materials were measured and compared. Metallographic observations and density tests were also conducted.
Little physical damage, as evidenced by surface roughening and cracking, was observed in the materials cycled in the inert gas. However, relatively severe damage occurred in those specimens cycled in laboratory air. Extensive surface roughening and cracking was observed. A decrease in density from that of the as-received material was also found. Tensile strength degradations greater than 50% were measured parallel to the fiber axis, while transverse strength reductions of as much as 77% were observed. Fibers extracted from specimens cycled in argon showed little or no strength decrease while the fibers extracted from air-cycled specimens had large strength reductions.
The observations of increased thermal cycling damage in air compared to argon were explained on the basis of thermal corrosion fatigue damage to the matrix and reaction of the fibers with the matrix and with the air.
The stresses and strains generated in a composite during thermal cycling were calculated. Their contribution to the damage sustained by the material was evaluated.
Thesis76.W458.pdf
11.43 MB
Adobe PDF
598b0b7fd67e572ae3555ab6b5db5aab