A study of the cold worked state and annealing behavior of the austenitic stainless steels
An investigation of the structural changes accompanying cold working and annealing treatments of seven austenitic stainless steels has been carried out. The materials studied included five laboratory prepared alloys and two commercial grades of austenitic stainless steels (AISI types 304 and 316). X-ray line profile analysis has been used to measure the stacking fault energies of the seven steels. Transmission electron microscopy combined with the x-ray line profile analysis was used to characterized the cold worked state of the steels. The recovery and recrystallization behavior of the steels were studied with a combination of transmission electron microscopy, hardness measurement, x-ray line profile analysis and measurements of electrical resistivity. The time-temperature-precipitation behavior of type 304 steel was also studied. The correlation between the equivalent chromium theory and the electron vacancy theory for predicting the stability of austenitic stainless steels with respect to sigma phase formation is discussed.
The stacking fault energies obtained from the seven austenitic steels range from 8 mJ/m2 to 68 mJ/m2; the results confirm the general trend that both Ni and C increase the stacking fault energy.
The results of transmission electron microscopy indicate that the dislocation arrangements are affected by the stacking fault energy. The dislocations tend to be arranged in planar arrays along their slip planes for steels of lower stacking fault energy. Dislocation arrangements are more random for steels of higher stacking fault energy. In no case studied was the stacking fault energy high enough to allow the cross slip necessary to generate a dislocation cell structure in which relatively dislocation free areas are surrounded by dislocation tangles.
The x-ray line profile analysis of the cold worked samples indicated that the particle sizes are reduced with increasing amount of deformation. The 304 steel with lowest stacking fault energy shows a smaller particle size (80 Å after 60% rolling) than the 316 steel (150 Å after 60% rolling) with highest stacking fault energy. The measured particle sizes fall into the range that has been found in other alloys which do not develop distinctive dislocation cells during deformation, but they are considerably smaller than for metals and alloys which develop a cell structure. These results are in qualitative agreement with the results of transmission electron microscopy.
Isochronal annealing of the steels revealed one major stage of resistivity recovery prior to recrystallization. This is believed to be primarily due to the annihilation of vacancies and formation of fine carbide precipitates. The TEM results indicate that no major rearrangement of dislocations takes place after short time aging at temperatures below 550°C. At a temperature of 650°C and above, one hour aging produced a noticeably recovered dislocation structure with the dislocation density reduced substantially. X-ray line profile analysis indicates that the microstrains decrease considerably after annealing at 550°c for 10 hours, which also indicates the annihilation of dislocations.
Recrystallized grains appear to be nucleated primarily by the migration of the former grain boundaries. The temperatures for the start of recrystallization are affected by the magnitude of the stacking fault energies through their effect on the cold worked dislocation structure and/or an effect of stacking fault energy on the amount of recovery prior to recrystallization. Recrystallization of the steels delayed substantially by a pre-aging treatment of 50 hours at 500°C. The effect is believed to be due to a decrease of stored energy by the annihilation of point defects and dislocations during the 500°C aging treatment. The precipitation of fine carbide particles on the dislocations and grain boundaries may also play a role.
The study of time-temperature-precipitation behavior of the 304 steel revealed that no intermetallic compound was formed after 4000 hours of aging. This is in excellent agreement with the prediction of equivalent chromium theory. The theory of electron vacancy numbers is inferior in predicting the formation of sigma phase in austenitic stainless steels as compared with the equivalent chromium theory. Modification is needed before the electron vacancy calculation can be applied to the system of austenitic stainless steels.
Thesis77b.Y446.pdf
15.35 MB
Adobe PDF
ac3b9ec9cbb97dc3f91f0a5185c58aa9